| Customization: | Available |
|---|---|
| Type: | Alloy Steel Bar |
| Standard: | AISI, ASTM |
Suppliers with verified business licenses
Audited by an independent third-party inspection agency
Cobalt Molybdenum HSS-Co 8 Round Bar, Flat Bar and Strip for Cutting Tools and Precision Dies
M42 is a cobalt-bearing, molybdenum-based super-hard high speed tool steel, standardized as ASTM A600 M42 (UNS T11342). The same grade is produced as HS2-9-1-8 under EN ISO 4957, as material number 1.3247 (S2-10-1-8) in the German system, as SKH59 in JIS G4403, as W2Mo9Cr4VCo8 in GB/T 9943, as BM42 in BS 4659 and as S500 in the Bohler range. With about 1.10% carbon, 9.5% molybdenum, 1.5% tungsten and 8% cobalt, it is the most widely used super-hard grade in the HSS-Co family.
The cobalt addition raises the tempering resistance of the martensitic matrix, so a correctly hardened M42 tool keeps a cutting edge at temperatures where M2 and M35 soften. Combined with a low vanadium content, the grade also grinds more easily than the vanadium-rich super-hard steels, which makes it practical for complex geometries such as form cutters, broaches and fine-pitch hobs.
FUSHUN METAL supplies M42 bars to cutting tool manufacturers, aerospace machining shops, gear and transmission plants, fastener and cold forming factories, die and mould builders and saw blade producers. It is selected wherever high cutting speeds, abrasive or heat-resistant work materials and long tool life are required.
| Standard System | Standard Number | Designation | Remark |
|---|---|---|---|
| USA (AISI / ASTM) | ASTM A600 | M42 | UNS T11342 |
| USA (ASME) | ASME SA600 | M42 | Boiler and pressure related orders |
| USA (Federal) | QQ-T-590 | M42 | Tool steel bar, federal class |
| Europe | EN ISO 4957 | HS2-9-1-8 | Also referenced as HS 2-9-1-8 |
| Germany | DIN / W-Nr. | 1.3247 | Old symbol S2-10-1-8 |
| Japan | JIS G4403 | SKH59 | Hitachi YXM42, Nachi HSD42 |
| Korea | KS | SKH59 | Same designation as JIS |
| China | GB/T 9943 | W2Mo9Cr4VCo8 | ISC T72948 |
| United Kingdom | BS 4659 | BM42 | Also listed as HS2-9-1-8 |
| France | NF A35-590 | HS2-9-1-8 | AFNOR tool steel list |
| Sweden | SS | 2716 | Scandinavian equivalent |
| Russia | GOST 19265 | R2AM9K5 | Near equivalent, lower cobalt |
| Austria (producer) | Bohler | S500 | Producer designation |
No dedicated AMS sheet is issued for this grade; AMS 6491 covers the M50 bearing steel and is not an M42 equivalent. Aerospace orders are normally placed to ASTM A600 or QQ-T-590. Where a customer drawing cites SKH59, 1.3247 or S500, FUSHUN METAL confirms the cross reference against the full chemical and hardness requirement before production starts.
Aerospace and Defence
Drills, reamers and end mills for titanium alloys, Inconel and Hastelloy; form tools for turbine blade roots; countersinks and hole deburring cutters for structural components.
Automotive and Gear Making
Gear hobs, shaper cutters, gear shaving cutters, spline broaches for transmission shafts, cold extrusion punches, thread rolling dies and M16 hexagon trimming dies.
General Metal Cutting
Twist drills, taps, threading dies, milling cutters, slitting saws, cold saw blades, lathe tool bits, boring tools and parting-off blades.
Fastener and Cold Forming
Header dies, nut forming punches, socket head punches, trimming dies, TiN-coated punches and wear plates for high-cycle forming lines.
Powder and Die Casting Tooling
Powder compaction dies, die inserts, extrusion rams, engraving cutters and precision punch components exposed to heavy mechanical wear.
Wood, Plastic and Recycling
Planer knives, router bits, profile cutters, chipper and shredder blades, and knives for abrasive board and composite materials.
| Product Form | Process | Size Range | Tolerance / Note |
|---|---|---|---|
| Round bar | Hot rolled | Dia. 16 - 350 mm | As rolled, plus tolerance |
| Round bar | Forged | Dia. 130 - 800 mm | Forging ratio above 6 |
| Round bar | Cold drawn / peeled / ground | Dia. 3 - 100 mm | h9, h10, h11 available |
| Flat bar | Hot rolled | 5 - 100 mm thick, 44 - 310 mm wide | Milled edge on request |
| Flat / square block | Forged | Up to 800 x 800 mm | Sawn or rough machined |
| Strip / coil | Cold rolled, annealed | 0.5 - 6.0 mm thick, 10 - 300 mm wide | Slit edge or round edge |
| Wire / drill rod | Cold drawn | Dia. 0.3 - 13 mm | Coil or straight length |
| Length | Cut to length | 1000 - 6000 mm | Fixed or random length |
Delivery Condition
Hot rolled or forged bars are delivered annealed and spheroidized. Cold drawn, peeled and ground bars may be delivered annealed, cold worked, or quenched and tempered where the drawing requires it. Annealed hardness is held at or below 269 HB; cold drawn bars are held at or below 285 HB and cold drawn plus annealed bars at or below 277 HB. Stress relieving at 600 - 700 degrees Celsius is offered on cold finished sizes.
Surface Condition
Black as rolled, rough turned, peeled, centreless ground, polished or bright drawn. Ground and peeled bars are supplied free of decarburization within ASTM A600 limits. Each bar is chamfered at both ends, marked with heat number and grade, bundled with steel strap, wrapped in VCI paper and packed in seaworthy wooden crates suitable for container shipment.
The melt analysis below follows the four specifications most often cited on customer drawings: ASTM A600 for M42, EN ISO 4957 for HS2-9-1-8 (1.3247), JIS G4403 for SKH59 and GB/T 9943 for W2Mo9Cr4VCo8. FUSHUN METAL melts to the tighter inner window shown in the last column, which keeps cobalt and molybdenum in the upper half of the range for stable red hardness from heat to heat.
| Element | ASTM A600 M42 | EN ISO 4957 HS2-9-1-8 | JIS G4403 SKH59 | GB/T 9943 W2Mo9Cr4VCo8 | FUSHUN Typical |
|---|---|---|---|---|---|
| C | 1.05 - 1.15 | 1.05 - 1.15 | 1.05 - 1.15 | 1.05 - 1.15 | 1.09 |
| Si | 0.15 - 0.65 | max 0.70 | max 0.70 | 0.15 - 0.65 | 0.30 |
| Mn | 0.15 - 0.40 | max 0.40 | max 0.40 | 0.15 - 0.40 | 0.28 |
| P | max 0.030 | max 0.030 | max 0.030 | max 0.030 | 0.018 |
| S | max 0.030 | max 0.030 | max 0.030 | max 0.030 | 0.006 |
| Cr | 3.50 - 4.25 | 3.50 - 4.50 | 3.50 - 4.50 | 3.50 - 4.25 | 3.90 |
| Mo | 9.00 - 10.00 | 9.00 - 10.00 | 9.00 - 10.00 | 9.00 - 10.00 | 9.50 |
| W | 1.15 - 1.85 | 1.20 - 1.90 | 1.20 - 1.90 | 1.15 - 1.85 | 1.50 |
| V | 0.95 - 1.35 | 0.90 - 1.30 | 0.90 - 1.30 | 0.95 - 1.35 | 1.15 |
| Co | 7.75 - 8.75 | 7.50 - 8.50 | 7.50 - 8.50 | 7.75 - 8.75 | 8.10 |
| Ni | max 0.30 | - | - | max 0.30 | 0.12 |
| Cu | max 0.25 | - | - | max 0.25 | 0.08 |
Values are percent by mass. Iron is the balance. Carbon, sulphur and phosphorus are verified by combustion analysis and the alloying elements by optical emission spectrometry on every heat.
The reference heat treatment used for the values below is: preheat in two steps at 450 - 500 degrees Celsius and 850 - 900 degrees Celsius, austenitize at 1180 degrees Celsius, quench in oil or in a salt bath held at 540 - 560 degrees Celsius, then air cool and temper three times at 540 degrees Celsius for one hour each. This route gives a secondary hardening peak without grain coarsening.
| Condition | Hardness | Tensile Strength Rm | Yield Strength Rp0.2 | Elongation A5 | Impact Energy |
|---|---|---|---|---|---|
| Annealed, as delivered | max 269 HB | 850 - 950 MPa | 550 - 650 MPa | 8 - 12 percent | 25 - 35 J |
| Cold drawn, as delivered | max 285 HB | 950 - 1100 MPa | 650 - 780 MPa | 6 - 10 percent | 20 - 30 J |
| Hardened 1180 C and triple tempered 540 C | 66 - 70 HRC (67 - 69 typical) | 2400 - 2800 MPa | 2200 - 2500 MPa | 1 - 2 percent | 10 - 18 J |
| Hardened and held at 600 C | 58 - 60 HRC | - | - | - | - |
| Transverse rupture at 67 - 68 HRC | - | 3000 - 3600 MPa | - | - | - |
Typical values for guidance only and not for design purposes; results vary with section size, austenitizing temperature and tempering programme. Compressive strength at 67 HRC is in the range of 3900 to 4500 MPa and elastic modulus is about 220 GPa.
Annealing: heat to 860 - 880 degrees Celsius, hold two to four hours, then cool in the furnace to 600 degrees Celsius at 20 - 30 degrees per hour before air cooling. Stress relieving: hold at 650 - 750 degrees Celsius and cool in the furnace. Hardening: salt bath 1170 - 1190 degrees Celsius or controlled atmosphere furnace 1180 - 1200 degrees Celsius; quench in oil, salt at 540 - 620 degrees Celsius, or gas. Tempering: 540 - 560 degrees Celsius, at least three cycles, with straightening between 200 and 450 degrees Celsius where required. For simple high hardness tools, austenitize at 1190 - 1200 degrees Celsius and temper at 530 - 540 degrees Celsius for 67 - 69 HRC. For complex shapes such as milling cutters and taps, use 1170 - 1190 degrees Celsius with tempering at 550 - 560 degrees Celsius for 66.5 - 67.5 HRC and better toughness.
Red hardness is the key advantage. Against M2, this grade keeps roughly three to four HRC more at 550 to 600 degrees Celsius, which translates into cutting speeds 40 to 80 percent higher and tool life several times longer on heat resistant alloys.
FUSHUN METAL melts M42 in an electric arc furnace followed by ladle refining and vacuum degassing, with electroslag remelting available for tool makers who need the lowest inclusion level. Vacuum degassing holds hydrogen low and reduces the risk of flakes, while ESR refines the solidification structure and gives a cleaner, more homogeneous ingot. Ingots are forged and rolled with a controlled reduction schedule to break up the as-cast carbide network, then spheroidize annealed so the bar arrives soft enough for machining and stable during hardening.
Quality control runs under an ISO 9001 certified quality management system. Every heat is checked by optical emission spectrometry and combustion analysis, and the carbon, cobalt, molybdenum and tungsten results are reported on the certificate. Carbide distribution and banding are rated against SEP 1615 and ASTM A561. Bars are 100 percent ultrasonic tested to SEP 1921 or GB/T 6402, and decarburization depth is verified within ASTM A600 limits on the finished size. Annealed hardness, dimensional tolerance and straightness are inspected before release.
Each shipment leaves with an EN 10204 3.1 mill test certificate showing heat number, grade, dimensions, chemical analysis, hardness and ultrasonic result, giving full traceability from finished bar back to the melt. Third party inspection and additional testing are accepted on request, and our metallurgists will review the customer heat treatment route and recommend austenitizing and tempering parameters matched to the tool geometry and section size.
What condition and surface finish do you supply? Round, flat and square bars are supplied annealed and spheroidized, or cold drawn, peeled, turned, ground and polished. Annealed hardness is at or below 269 HB, cold drawn at or below 285 HB. Bars are cut to length, chamfered, marked with heat number and packed in seaworthy wooden crates.
Which heat treatment do you recommend for cutting tools? Preheat in two steps at 450 - 500 and 850 - 900 degrees Celsius, austenitize at 1170 - 1200 degrees Celsius, quench in oil or salt at 540 - 560 degrees Celsius, then temper three times at 540 - 560 degrees Celsius. Expect 66 to 70 HRC. Use the lower austenitizing range for complex shapes and the higher range with low tempering for maximum hardness.
Can you replace SKH59, 1.3247, S500 or W2Mo9Cr4VCo8? Yes. FUSHUN METAL produces all of these as one grade family and confirms the cross reference against your drawing before production. We also support mixed sizes in one container, small trial quantities, EN 10204 3.1 certification and third party inspection.
FUSHUN METAL supplies M42, 1.3247, SKH59, S500 and W2Mo9Cr4VCo8 high speed steel bars with ISO 9001 certified quality control, full heat traceability and EN 10204 3.1 certification. Send us your grade, standard, dimensions, quantity and delivery condition and we will return a quotation with a recommended heat treatment route for your application.